Fixes & Fractures

By some miracle, I have been paddling kayaks on rivers and seas and in the open ocean for almost 40 years. I have never broken a kayak. I’ve scraped rocks and watched friends broach and bail out as their boat wrapped around rocks or trees and bent (plastic) or splintered (composite). I’ve seen friends piton in sea arches that knocked golf-ball-sized holes into bows, but I have never had a broken kayak of my own, composite or plastic, until 2023. Of course, it had to be the nicest, most expensive kayak I have ever owned, one so sweet I call her “Honey”. She’s a Carbon/Kevlar Sterling Design Grand Illusion, my most valuable possession, so repairing her was a cause for care.

Fixes & Fractures

As the owner of a remote kayak outfitting and guide service, I cannot simply send complex or simple repairs to a shop to be taken care of. I have to be able to attend to all the repairs that come up due to either client neglect or simple wear and tear. I’ve become somewhat known as a fixer of broken kayaks and their bits in my little town of 8,000, where there are about 1,000 kayaks.

I have had quite a lot of experience working with composites and repairing broken kayaks. In the late ’90s, I worked in a “glass” shop making helmets and “squirt” boats (sub-surface white water kayaks), so I have a pretty good knowledge base for working with resins and fiber. I’ve picked up the plastic repairs as I’ve gone along out of necessity,

In the last year, I have refinished three boats, fixed “antique” rudder mounts, replaced rudder and skeg cables, patched full-thickness breaks, and made structural repairs on about a dozen composite and plastic kayaks.

Fixes & Fractures

Here are some things to keep in mind:

All the fumes from the resins for plastic or composite repairs are highly toxic. Wear proper protective equipment, good dust masks for sanding, respirators for resin, epoxy and gel coat, long sleeves and trousers, eye protection, and the right gloves.  All the resins, etc., are heat-sensitive. They work best in temperatures above 70 degrees F and 21 degrees C. BUT the hotter it is in your work environment, the faster the hardener activates. In colder temperatures, the amount of hardener in your composite repairs and gel coats can be increased to heat the mix, but it makes for a more brittle repair.

Fixes & Fractures

Let’s talk materials for plastics:

Today, you can get several different systems for plastic repairs: JB and/or Devcon Plastic Weld, JB Water Weld and West Systems Plastic Repair Kit. Of the plastic weld, I prefer the Devcon as it hardens up faster.

I use both for different fixes. For my HTP fixes, I like the West Systems because it spreads and works more easily, especially with fiber. Using fiber is not necessary, but in talking to different manufacturers in the US and Canada, it is what is recommended by their repair gurus. The JB Weld works better for rotomolded boats and for broken bits like old rudder mounts.

If you are working on a break on an HTP kayak, the first thing to do is to drill a small hole at either end of the break to prevent the cracks from spreading after repair. Then, get the edges realigned however you can. This includes force, sanding, and any other method that works. Carefully using a heat gun is a good help. Then, I file or grind with a Dremel a little groove on the inside of the boat along the length of the break for the epoxy to fill.  Once this is done, I clean the surface well with alcohol or toluene. Alcohol works just about as well and is much more environmentally friendly. Tape a frame around the break that gives you a 2-inch or 5-cm radius, and cut a piece of light glass to shape, rounding off the corners. Mix the resin and hardener and smear a layer over the framed section using a spatula or spreader. Place your cloth atop it and work the mix into the cloth. I use my gloved hands for this and am careful not to pull too hard on the fiber. This stuff dries quickly in any heat, so ensure you have everything ready to go before mixing! Repeat the process on the outside. In some people’s view, this is overkill, but I do it anyway. Sand edges flush and paint if desired.

The JB Weld has highly toxic fumes, so beware. It’s much less spreadable than the West Systems and tends to glob. I use it mostly on rotomolded boats or as filler for punctures in the hull or deck of HTP or composites using it like wall filler. Once hardened, I sand it down and put a fiber repair over it.

Fixes & Fractures

Composites:

I do all my work on composites by hand without power tools. It is slower but prevents me from going too deep into the layers. You need to be especially careful not to sand into Kevlar.

Sand both outside and inside in a 2-inch or 5-cm radius all the way around your break or puncture. Clean it really well, as for plastics. Prep your cloth carefully, as per plastics.

Composite work is more delicate and requires a lot of attention to detail. Your MEKP hardener is the most toxic substance you will work with. You must wet the cloth thoroughly but not excessively. Depending on the location of the work area, I will either spread the resin mix before putting the cloth down or wet the cloth first. I do the latter in places where the resin will likely pool.

Aside from the epoxy you use, the only real difference in the composite process is that you should do two layers inside and one on the outside.

Fixes & Fractures

In the Field Repairs:

The JB WATER WELD and the Devcon Plastic Weld are my instant field repairs. Both of these products can be used on any material with quick and lasting results. The water weld can be used in water if ever necessary. In the past, I carried a full fiberglass repair kit complete with resin, hardener, and cloth, and I have needed to make fairly serious repairs on friends’ kayaks while far from town. It was difficult and time-consuming and required drying the area thoroughly with heat from a fire while under a tarp in the pouring rain of an Olympic Peninsula early winter storm. I still carry a full glass repair kit if I am on an extended tour, but they are bulky. I have included a picture of my field repair kit for my shorter (under two weeks) trips around Sitka. It has everything I need to make a temporary repair of my carbon Kevlar kayak and a full repair on HTP or rotomolded kayaks.